| Test |
GM Specification |
Rating |
| Adhesion |
GM 9502P |
Pass |
| Conical Mandrel |
GM 95003 P |
Pass |
| Film Thickness |
ASTM D1186 |
0.6 mils |
| Reflectometer (60 degrees) |
ASTM (D523) |
87 |
| Humidity and Tape Adhesion (96 hours) |
GM 4465P (7/95) and GM 9071P |
No adhesion loss - Pass |
| Salt Spray (336 hours) |
GM 4298 (6/97) |
1.9 mm - Pass |
| Chip resistance |
GM 9508P |
GM 7 - GM 8 |
| Dime Scrape |
GM 9506P |
No brittleness |
| Gasoline Resistance - Dip |
GM 9501P (97) |
Pass |
| Gasoline Resistance - Puddle |
GM 9500P (98) |
Pass |
| Oil Resistance - Dip |
GM 4350M - 5.3.11 |
No marring |
| Oven Aging |
GM 9504P (90) |
No abnormal results |
| Note: Initial Cured Film Performance on ACT Cold Rolled Steel Panels. Performance on Production Parts or Other Substrates May Vary. |
| Test |
Ford Specification |
Rating |
| Adhesion |
FLTM BI 106-01 |
Grade 0 -Pass |
| Film Thickness |
FLTM BI 117-01 |
0.6 mils |
| Salt Spray (480 hours) |
FLTM BI 103-01 |
1.3 mm - Pass |
| Pencil Hardness |
|
>4H |
| Water Immersion 24 hours |
FLTM BI 104-01 |
Grade 0 - 0% Removal |
| Water Immersion 240 hours |
FLTM BI 104-01 |
Grade 0 - 0% Removal |
| Chip Resistance |
SAE J400 |
5B - Pass |
Abrasion Resistance
1000 Cycles |
FLTM BN 108-02, CS #10 |
Pass (at 0.8 mils) |
| Mar & Scratch Resistance |
FLTM BN 108-04 |
Pass |
| Resistance to Water/Soap Spotting |
FLTM BI 113-01 |
Pass |
| Fogging Resistance |
FLTM BO 116-03 |
Pass |
| Cleaning Solution Resistance |
FLTM BI 107-01 |
Pass |
| Note: Initial Cured Film Performance on ACT Cold Rolled Steel Panels. Performance on Production Parts or Other Substrates May Vary. |
| Test |
Chrysler Specification
|
Rating |
| Adhesion |
463PB-15-01 |
Grade 5B -Pass |
| Film Thickness |
LP463PB-42-01 |
0.6 mils |
| Humidity (240 hours)
|
463PB-09-01 |
No Blister - Pass |
| Humidity (480 hours) |
463PB-09-01 |
No Rust - Pass |
| Salt Spray (336 hours) |
463PB-10-01 |
1.9 mm - Pass |
| Solvent Rub |
463PB-07-01 |
Pass |
| Gravel |
463PB-39-01 |
Pass |
| Note: Initial Cured Film Performance on ACT Cold Rolled Steel Panels. Performance on Production Parts or Other Substrates May Vary. |
| Test |
ASTM Specification |
Rating |
| Adhesion |
ASTM D3359 |
Grade 5B -Pass |
| Conical Mandrel
|
ASTM D522 |
Pass |
| Film Thickness |
ASTM D1186 |
0.6 mils |
| Reflectometer (60 degrees) |
ASTM D523 |
87 |
| Humidity (240 hours) |
ASTM D2247 |
No Blister - Pass |
| Humidity (480 hours) |
ASTM D2247 |
No Rust - Pass |
| Salt Spray (336 hours) |
ASTM B117 |
1.9 mm - Pass |
| Reverse Impact (160 in .lbs.) |
ASTM D2794 |
Pass |
| Pencil Hardness |
ASTM D3363 |
>4H |
| Gravelometer |
SAE J-400 |
6A |
| Note: Initial Cured Film Performance on ACT Cold Rolled Steel Panels. Performance on Production Parts or Other Substrates May Vary. |